A threaded flange joins pipe to pipe, or pipe to equipment, by screwing the pipe into a tapped bore instead of welding it. There is no hot work, no weld inspection, no post-weld heat treatment, and the joint can be broken and remade with wrenches. That is why threaded flanges hold their place on utility headers, instrument and sample lines, small-bore drains and vents, and anywhere a plant restricts hot work or a shutdown window is too short for welding.

The trade-off is that the thread becomes part of the pressure boundary: the seal is interference between two tapered threads plus sealant. A flange with the wrong thread form, or one made up badly on site, leaks in a way that no amount of bolt torque will fix. This guide covers what the standards define, what they leave to the purchase order, and where a threaded joint stops being the right answer. Acceptance criteria come from the applicable standard edition, the project specification and a qualified engineer.

Two stainless steel flanges with raised faces, tapered hubs and eight bolt holes standing on a red surface
Stainless steel flanges with raised faces and eight-bolt drilling. A threaded flange keeps this outside diameter, thickness and bolt circle, but the bore is tapped instead of prepared for welding.

What a Threaded Flange Is, and What It Is Not

In ASME B16.5 a threaded flange is a full flange: the same class designation, rating basis, bolt circle and facing options as the weld neck or blind type in the same standard. Only the bore changes, carrying an internal pipe thread instead of a weld preparation. Three consequences belong in every enquiry.

It has two independent sizes. One is the thread size, the other fixes the body dimensions. They match on a straight threaded flange and diverge on a reducing one, so the difference must be written down.

The thread seals the pipe, not the flange pair. The joint between two flanges still needs a gasket and bolting. A weep at the thread is often read as a gasket problem, so the faces get re-torqued while the leak sits behind the pipe.

The joint is made up, not tightened. Thread engagement, sealant and alignment decide whether it is tight. Bolt torque only compresses the gasket between the two faces.

NPT, BSPT and BSPP: What Actually Differs

Two thread families dominate, and they are not interchangeable. Both tapers are 1:16, so a wrong pair often starts by hand and then leaks under pressure – the worst failure mode, because it passes a quick site check.

Thread Standard, form and how it seals
NPT ASME B1.20.1, 60 degree thread angle, 1:16 taper. Seals by interference of the tapered threads plus sealant. The default on B16.5 threaded flanges in North American practice.
BSPT (R) ISO 7-1, 55 degree Whitworth form, 1:16 taper. Also seals on the threads. Common on European and Asian projects and on imported equipment.
BSPP (G) ISO 228-1, 55 degree parallel thread. Tightness is deliberately not made on the thread: the joint needs a face seal, bonded washer or O-ring. A tapered thread is not a substitute.

The forms differ in more than flank angle: at 1 inch nominal NPT has 11.5 threads per inch and BSP has 11, so the threads never seat over their full length.

Internal pipe thread cut into the bore of a stainless steel cylindrical pipe coupling
An internal pipe thread in a stainless steel coupling. The same thread form is cut into the bore of a threaded flange, and its condition – crests, roots, taper, cleanliness – decides whether the joint seals.

Where the drawing is silent, do not default on the supplier’s behalf. State thread family, standard and edition, and whether the bore is gauged: a flange with the right class and the wrong thread is scrap.

Where a Threaded Joint Is the Wrong Answer

A tapped bore removes wall section, the seal depends on thread interference rather than a full-penetration weld, and every make-and-break consumes thread. Treat these as stop signs unless the project specification says otherwise:

Codes commonly limit threaded joints to small bore and exclude them from severe cyclic duty; the limits sit in the code edition and project specification, not in a supplier’s general statement.

Writing the Enquiry So the Flange Can Be Made

Most threaded flange problems are order-entry problems. This list is the minimum that lets a manufacturer build the part without guessing:

When comparing suppliers, ask each to quote against the same list; otherwise the lowest price is often the one that silently dropped the gauging.

Materials, Galling and Seal Welding

Forged stainless flanges are normally ordered to ASTM A182/A182M, which covers forged or rolled alloy and stainless flanges for pressure service and ties each grade to its heat treatment and mechanical properties. 304L suits benign duty, 316L where chlorides are present, and duplex grades where chloride stress corrosion cracking or higher strength drives the choice. Match the flange grade to the pipe; a mismatched couple accelerates corrosion at the thread.

Austenitic stainless threads gall. Two clean 316 surfaces can pick up and seize before the joint seats, and a seized small-bore joint usually ends with the pipe cut out. A service-appropriate lubricant, slow make-up and no repeated re-tightening reduce the risk; avoid products that introduce chlorides.

Seal welding is the usual answer when the joint must be permanently tight. It is still a weld: qualified procedure and welders are needed, and on stainless steel the heat-affected zone must be cleaned and passivated. Some specifications prohibit seal welds because they remove the maintainability that justified the threaded joint, so confirm before quoting.

Making Up and Testing the Joint

Site practice decides more outcomes than the drawing does. A workable sequence:

  1. Inspect and clean both threads, remove caps and check the bore for swarf.
  2. Apply sealant to the male thread only. With PTFE tape, wind it in the thread direction and leave the first thread bare so no tape enters the bore.
  3. Engage by hand for the first turns. If it binds immediately, stop – the thread is wrong, damaged or dirty.
  4. Tighten with a wrench on the flange body, not by turning the pipe, so the joint is not over-torqued or distorted.
  5. Check that the faces come up parallel. If they do not, do not unscrew the joint to line up bolt holes: back-turning breaks the seal. Rework the piping.
  6. Fit the gasket, bring the bolts up in a cross pattern and torque to the project value for that gasket and bolting.
  7. Pressure test as specified and inspect the thread, not only the faces, for weeping.

Inspection on Receipt and Before Start-Up

A threaded flange can be checked quickly. Visually, the thread should be continuous and free of tears, laps and cross-threading, with no tool marks across the crests. The bore should be clear through, and the facing free of radial marks that would create a leak path.

Dimensional checks cover outside diameter, thickness, bolt circle, hole diameter and facing finish. Threads are verified by gauge: plug and ring gauges for NPT, limit gauges per the ISO 7 verification method for taper threads. Marking should identify size, class, material and manufacturer, and agree with the certificate.

Before start-up, confirm every threaded connection is made up to the specified engagement, the sealant suits the process, and seal-welded joints have been cleaned and passivated where required. A joint that weeps on hydrotest will not improve with temperature.

Frequently Asked Questions

Are NPT and BSPT threads interchangeable?

No. NPT is 60 degrees to ASME B1.20.1 and BSPT 55 degrees to ISO 7-1, and at the same nominal size the threads per inch differ. A mixed pair may assemble part way, then leak.

What pressure class does a threaded flange need?

The class is a rating category, not a working pressure. Allowable pressure depends on material group and design temperature through the rating tables in ASME B16.5. Take the class from the line’s design conditions and the project specification.

Can a threaded flange be seal welded?

Yes, where the project permits it and a qualified procedure is used. It makes the joint permanent, and on stainless steel the weld zone then needs cleaning and passivation.

Why do stainless steel threads seize during make-up?

Galling. Clean austenitic surfaces under pressure can pick up and weld together at the thread. A suitable lubricant, slower make-up and avoiding repeated re-tightening reduce the risk.

Does a threaded flange still need a gasket?

Yes. The thread seals the pipe into the bore; the joint between two flanges is still gasketed and bolted, with the same facing and gasket rules as any flange of that class.

Can I use a threaded flange on a large line?

Rarely sensible. Above small bore the bending moment at a screwed joint grows faster than the wrench can compensate, and most codes and owner specifications limit threaded joints by size and service.

Ordering Threaded Flanges Without the Rework

The part is simple: a rated body with a tapped bore. What fails is the specification around it – the thread family left to the supplier, the facing assumed, the seal weld discovered after delivery. Write thread, class, facing, material, seal weld decision and inspection into the enquiry, then check marking and thread on arrival.

If you are specifying threaded flanges for a small-bore package, send the line list with size, class, thread standard, facing and material, and we will quote against it. Start from our pipe flange and weld neck flange ranges, or use the contact page to send the details for review.

Technical information in this article is general. Final selection, pressure rating and acceptance criteria must be confirmed against the applicable standard edition (ASME B16.5, ASME B1.20.1, ISO 7-1, ISO 228-1, ASTM A182/A182M), the project specification and by a qualified engineer.